Troubleshooting Poor Edgeband Adhesion - Woodweb

11, Aug. 2025

 

Troubleshooting Poor Edgeband Adhesion - Woodweb

Troubleshooting Poor Edgeband Adhesion

Temperature and priming could be the culprits when PVC edgebanding doesn't stick well. April 12,

Question
I've noticed that occasionally when I peel a piece of edgebanding off of a panel that I've run through my Brandt KD55, the adhesion is poor. The glue line looks fine and solid, but very little glue remains stuck to the banding when I pull it off. Other times (within the same batch), the bond is fine, and the tape pulls the glue and parts of the panel core (melamine) with it.

View Details

I'm using a good brand of glue, working within the recommended temp range. Machine is set for the correct thickness edgeband. I don't believe that it's bad edgeband, as it's happened with a few different rolls. Not sure what's causing this.

Forum Responses
(Cabinetmaking Forum)
From contributor D:
The glue is most likely too cold when the banding is applied to the board, thus poor adhesion. There are also a few other factors that could be in play. Is your banding material laminate? Also, what is the ambient temperature in the shop when you are having these problems? If the board material is cold when the glue is applied, you will get poor adhesion.


From contributor S:
How are your pieces cut? A shop I did some work for had an issue with poor edgeband adhesion on pieces cut by their CNC, on some of the coarser particle core material. The CNC was losing the core, so the edgeband was easily removable. They tried to get a denser core material and on the coarser material, they started blowing the loose material out with air pressure. I think this resolved most of their issues.

From contributor P:
You said tape, right? PVC? There are 4 things that come to mind to check.

1) If you are working with PVC, you could be having a problem with poor primer on the tape or skipped sections where there is no primer at all. Hot melt will not adhere very well to unprimed PVC.

2) The second thing is glue temperature. With PVC it's not as critical to have perfect glue temperature as with HPL, but there is still a need to be reaching at least 180c to 200c (with a machine the speed of a KD55). Check the element at the top of the glue roller housing to make sure it is working.

3) Do you have proper flotation with the glue station? If you do not see the glue system ease back when the leading edge of the panel contacts it, then you are not sure you are making good contact between the roller and panel edge. The proper kickback of the glue system should be around 1/16". Then when the panel leaves the roller, you should see the glue system return back to home position. Your pot should be spring loaded and thus swivel slightly.

4) Do you have proper flotation of the pressure station rollers? Once again you should see the rollers kick-back slightly when the panel edge comes in contact with each of them. You can have board, glue and tape, but if you have no pressure you will not achieve good bond. The rollers must be seen to return to home position once the panel exits the pressure station. Too much pressure on the rollers will push the panel material away from the correct sight line that the edge started at. You should be able to take your hand and pull each roller back without too much effort. It takes very little pressure to bond edging if all settings and material is correct.

Does your panel material have a dog leg cut when you lay them on a perfectly flat surface? This could cause the center of the panel to not get pressure if the rollers do not have enough movement.


From contributor J:
All good stuff so far. I'd throw in that on my Holz-Her, all else being equal with the banding, panel and straight edge quality, the biggest culprits seem to be temperature and glue brand. I used Jowat for years with satisfactory results, but I had to fiddle with the temperature pretty regularly, especially in the winter months to compensate for cold panel stock. I found that Dorus has better overall adhesion and is less fussy that I have the temperature exactly right. Good bit more expensive, but I don't worry about my banding coming off!

From the original questioner:
All good information - thanks very much. I think the issue is, in fact, temperature related. From what I can tell, the pieces of banding that are pulling off easily are those that are being run through the bander first, immediately after it has come up to temperature. The temp readout is saying that the machine is up to temp, but it seems this isn't the case.

I've let the machine marinate for a few minutes after it comes up to temp, with better luck. I've also turned the temp up from 190 to 210, which I'd rather not have to do, but at this point will do for the peace of mind.

Still not clear why the machine isn't always up to temp when it says it is. All the heaters in the glue pot and tower have been replaced recently, so I don't think the issue is there. The glue gate moves very freely, which leads me to believe that heater is working fine (it had failed at one point and the glue gate was very stiff).


From contributor C:
What is the air and board temperature when you have the problems? Sounds like a pre-cure issue, not a glue temp issue. If it's a pre-cure issue, then increasing the glue temp will not solve the problem. I also recommend Dorus over Jowat glues when it's cold.

From the original questioner:
Using Dorus glue, shop temp is 55 degrees. Most pieces bond very well, it's just some that occasionally don't, even in the same batch of pieces.

From contributor C:
Is it colder than that overnight? The parts could still be colder than 55. You should get a laser pyrometer to check the actual part temp. When it gets cold we direct a flow of kerosene heater hot air across the edges of the parts before they are banded. We also store the PVC in the office to keep it warm.

From contributor J:
55 is a bit chilly for banding. I have pointed that kerosene heater at the front end (gluing area) of my bander as well as the parts on occasion in the morning and heated up the whole thing. Set it far enough back so it won't get dangerously hot, and so you don't thermally shock the metal, but so that it will warm up reasonably quickly. Give it 20-30 minutes to warm up all the machine metal. Also, I have to let my machine simmer at temp for a few additional minutes on the first run after it is that cold, or run a few test pieces to get the glue flowing good. Might bump your glue temp up 5 degrees or so as well. Better yet, keep your shop above 60 degrees.

From contributor L:
Our bander has an optional hot air blower that blows on the glue line between the application roller and the first pressure roller. When no banding is present the flow is redirected up away from the machine. Works good. We use Dorus with a chain speed of 18meters/min. You can probably get the hot air blower as an optional kit from Stiles.

From contributor A:
Our bander has a heated shoe before the dosing wheel to warm the board. Check the Knowledge Base - I think there was a thread about adding this feature with parts from Grainger.

From contributor V:
What Dorus product is everyone using? We are using Jowat and are having issues with our 1/8" solid wood edging. Mainly white oak and maple. We sand the back side with 36 grit and have also tried using the primer, and still get edges falling off. I have tried Dorus in the past and it didn't seem much to help.

From contributor L:
Ask Dorus. The appropriate adhesive varies with your chain speed and material. While you're at it, get a jug of their primer - good for wood or HPL.

Edge banding - some common FAQs - Glue Sticks, Guns, Dots & Hot ...

So, you’re running Henkel PUR, PO, PP or EVA hot melt adhesives for edge banding, edge lipping, edge sealing, soft forming or straight line gluing and therefore already recognise and demand the highest quality and performance from your adhesive.

Q: What types of glues are most commonly used in edgebanding?

A: Ethylene Vinyl Acetate (EVA) and Polyurethane reactive adhesives (PUR) hot melt adhesives are the most common. Polyolefin (PO) and polypropylene (PP) hot melts are also available.

Q: Can you describe the process of applying glue for edgebanding? 

A: Glue is put into the glue pot and melted to the specified temperature. Once this is reached it travels to the roller which has been adjusted to the optimal coat weight. The board passes through but does not touch the roller. A guide plate is set to ensure no contact is made between the board and the roller. Edging tape is passed through and contact between the board, glue and edging is made through the pressure rollers. The glue will lose its heat and materials are bonded. 

Q: What is the advantage PUR hot-melt adhesives for edgebanding?

A: It’s universally accepted that EVA is the easiest of all to use but comes with disadvantages where the end product is likely to be subjected to steam, heat, or moisture. Polyolefin adhesives fare better and also provide better stability when melting. But, when a watertight, heat-resistant bond is required, nothing is on the market to beat the performance of a Polyurethane reactive (PUR) adhesive.

Q: Are there certain types of glue better suited for edgebanding certain materials?

A: EVA, PO and PUR adhesives are compatible will all types of cores boards and edging material: veneer, melamine, polyester, HPL, PVC, ABS and PP

Q: How does the type of glue used affect the durability and aesthetics of the edge band?

If you want to learn more, please visit our website chimeda.

A: PUR adhesives are used if finished products are subjected to moisture, high heat or chemicals. This increases the durability of the finished product. Tight joints and zero glue lines are achievable. Good results can be achieved with EVA unfilled adhesives provided the correct type of EVA for the application is used.  

Q: EVA hot melt adhesives Filled or Unfilled?

A: Technomelt KS 220/1 and Technomelt KS 611 are both filled EVA edgebanding hot melt adhesives, which are easy to apply and offer exceptional performance with very high final bond strength.  Being filled EVA’s they offer the advantage of preventing stringing, whilst at the same time offering higher viscosity, which can be beneficial when applying to porous substrates such as chipboard. In the unfilled hot melt adhesive category, there is Technomelt Dorus KS 351.  This can be applied at lower coat weights, thereby minimising the glue line and achieving tighter joints, whilst offering high glue mileage and high final bond strength.  Technomelt KS 351 has really grown in standing to attain the status as the UK’s frontrunner and main contender when selecting an unfilled grade used by many of the well-known UK and European furniture manufacturers.

Q: What safety precautions should one take when handling and applying glue for edgebanding?

A: Always wear protective clothing: overalls or long-sleeve shirts, closed-toe shoes, heat-resistant gloves, and safety glasses or goggles. Keep long hair tied back, especially when this involves working with the hot glue pot. Molten adhesive can cause burns. Extraction is required when running PUR-based hot melt adhesive. Always read the safety data sheet (SDS) before use. You should always: Work in a well-ventilated area and run at the recommended operating temperature.

Q: How can one ensure an even application of glue for optimal edgebanding?

A: Running temperature, guide plate setting, and coat weight are all vital in achieving good glue coverage. The board must not touch the roller. You can reverse the edging tape or put the board through without edging (depending on the machine setup) to check glue coverage. 

Q: How do you clean up any excess or spilt glue during the edgebanding process?

A: Hot melt cleans are available to clean the outside of the machine (not glue pot) or adhesive overspill on boards. Technomelt Melt O Clean and Technomelt PURE are both good options. 

Q: Benefits of Polyolefin (PO) hot melt adhesives:

A: Polyolefin-based adhesives have better hydrolysis and heat resistance than EVA-based adhesives. They are easier to apply than PUR adhesive as EVA hot melts do not require a wax cleaner and also lower the formation of strings at the application unit, whilst providing better stability in the melting equipment, in comparison with standard EVA-based adhesives. Remember PUR based adhesives will always outperform both EVA or PO adhesives for heat and moisture resistance!

Q: How does the curing time of the glue impact the edgebanding process and final product?

A: The curing time of the glue can have a big impact on the manufacturing process and the quality of the final product. Ensure the glue is correct for your machine speed (m/min) and make sure the correct running temperature is followed. This may increase or decrease depending on working conditions. Glue drying too quickly or taking too long to go off will both result in bond failures. 

Q: Are there eco-friendly glue options for edgebanding? 

A: Markets are demanding more from adhesive technology. Sustainable and renewable adhesives along with Micro Emission are dominating the market. Technomelt 270-9 micro emissions PUR technology and Technomely 279-9 PUR adhesive based on renewable carbon-based raw materials making gluing kinder to the planet.

Q: Why use Micro emission PUR adhesives?

A: Micro emission PUR adhesives from Henkel, contain less than 0.1 % Isocyanate, therefore reducing the hazardous isocyanate-containing vapours by up to a staggering 90%!  Nobody likes warning labels and the fact that we can now eliminate this has huge benefits not only to ourselves but also for end users, whilst still providing them with a PUR adhesive used for bonding all commonly used edging materials; PVC, ABS, veneer and solid wood to core boards. With companies becoming increasingly mindful of health and safety are turning to ME adhesives to allow them to improve their operating procedures whilst at the same time reducing risk.  The solution is simple Henkel Technomelt Micro Emission adhesives (ME). These adhesives offer the same performance benefits that come with PUR technologies, but without the hazardous labelling, making it more environmentally friendly and safer for operators to handle.

Q: Do Henkel provide hot melt cleaners?

A: The Henkel name is quite rightly associated with quality and market-leading technologies, and this doesn’t purely apply to their adhesives, but also to their extensive range of hot melt cleaners, which cover everything from surface cleaning to system/application equipment cleaning.  Given that an effective cleaning process can make all the difference in meeting deadlines, maximising output and achieving daily goals, we are here to help set you on the right path and ensure you are getting the most out of your day. The right cleaner will bring you many operational benefits, ensuring consistent dispensing & bond quality, reducing downtime & maintenance, as well as prolonging the lifespan of application equipment.   Not to mention the peace of mind factor – there’s nothing better than being able to leave your equipment safe in the knowledge that the cleaning process has finished and therefore your edge bander will be all ready for the start of the next production run.  Whilst a good cleaning process is key for all adhesives, it is essential for PUR adhesives to prevent the glue from cross-linking. A good quality and appropriate cleaner used in the correct way can save hours of downtime over the lifetime of the edge bander by reducing the amount of time spent on the cleaning process, thereby maximising production time.  Streamlining the cleaning process is just as key as selecting the most appropriate and superior quality adhesive.

If you want to learn more, please visit our website PP Edge Banding.